First, the gloss is not good, the brightness is not enough
main reason:
1. The viscosity of UV varnish is too small, and the coating is too thin.
2. Excessive dilution of non-reactive solvents such as ethanol.
3. Uneven coating of UV oil.
4. Paper absorption is too strong.
5. The anilox roller is too thin and the oil supply is insufficient.
Solution: Properly increase the viscosity and coating amount of UV varnish according to different conditions of paper. A layer of primer can be applied to paper with strong penetration and absorption.
Second, poor drying, incomplete light curing, and sticky surface
main reason:
1. The intensity of ultraviolet light is not enough.
2. The UV lamp is aging and its intensity is weakening.
3. The UV varnish storage time is too long.
4. Too much diluent that does not participate in the reaction is added.
5. The machine speed is too fast.
Solution: In the case of curing speed requirements less than 0.5s, it must be ensured that the power of high-pressure mercury lamps is generally not less than 120w / cm. If necessary, add a certain amount of UV varnish curing accelerator to accelerate drying.
3. The UV varnish on the surface of the printed matter can not be coated or flowered
main reason:
1. The UV varnish has low viscosity and the coating is too thin.
2. The ink contains too much ink or dry oil.
3. The ink surface has crystallized.
4. There are many anti-sticking materials (silicone oil, powder) on the surface of the ink.
5. The glue roller is too thin.
Solution: When printing products that require UV glazing, appropriate measures must be taken to create conditions. When UV varnish is applied, it should be thicker. If necessary, the problem can be solved by applying primer or replacing special varnish.
4. UV coating has white spots and pinholes
main reason:
1. The coating is too thin.
2. The anilox roller is too thin.
3. Too much non-reactive diluent (such as ethanol) is added.
4. There is more dust on the surface of the printed matter.
Solution: The production environment and the surface of the printed matter should be kept clean and the coating thickness should be increased. A small amount of smoothing aid can also be added. For dilution, it is best to use reactive diluents that participate in the reaction.
5. Uneven coating on the surface, streaks and orange peel
main reason:
1. The viscosity of UV varnish is too high.
2. The coating roller is too thick and not smooth.
3. The pressure is not uniform.
4. The coating amount is too large.
5. Poor leveling of UV varnish. Solution: reduce the viscosity of UV varnish and reduce the amount of coating. The pressure is adjusted evenly. The coating roller should be ground and polished. Light leveling agent can be added.
Six, UN varnish adhesion is not good
main reason:
1. Crystallization of printed matter ink surface.
2. The auxiliary materials in the printing ink are not suitable.
3. The UV varnish itself has insufficient adhesion.
4. Light curing conditions are not suitable.
Solution: The printing process should consider the glazing conditions in advance. The printed product needs to be coated with primer to enhance adhesion.
7. UV varnish thickens and gels
main reason:
1. The UV varnish storage time is too long.
2. Varnish is not completely protected from light.
3. The storage temperature is too high.
Solution: Pay attention to the effective use period of UV varnish and store it strictly in the dark. The storage temperature is preferably 5 ℃ ~ 25 ℃.
8. Large residual odor
main reason:
1. Dry curing is not complete.
2. Insufficient UV light source or aging lamp.
3. The UV varnish has poor anti-oxygen interference ability.
4. Excessive addition of non-reactive diluent in UV varnish.
Solution: UV varnish must be dried and cured thoroughly. And to strengthen ventilation, if necessary, replace the UV varnish varieties.
After a hard working day, you went home, Pour a glass of wine, Seating on the bistro chair and table, peering ahead, find opportunities for encounter your mind.
Transform your outdoor space with our range of bistro tables, chairs & sets at golden eagle. We have something to suit every household - find charming, compact bistro tables for city balconies or large rattan armchairs for big back gardens so you can stretch out and read the paper under the sun.
· UV-resistant polyethylene environmental rattan
· Powder coated strong no rust aluminum tube
· Hard all kinds of tempered glass
· Cushions with 100% waterproof fabric.
If you have any questions, please contact with us directly. Outdoor Sofa Furniture are produced by Golden Eagle Outdoor Furniture With High Quality and Good Appearance. Welcome you can visit our Factory.For any inquiry,Please send mail directly to us.
Bistro Chair And Table,Garden Bistro Chair And Table,Patio Bistro Chair And Table,Rattan Bistro Chair And Table
Golden Eagle Outdoor Furniture Co., LTD. , https://www.gegardensets.com